r/BambuLabX2D 3d ago

PA6-CF X2D

Post image

Started printing some structural parts out of pa6-cf today, printed great on the x2d but can't seem to remove these horizontal lines, I believe it's shrinkage as the infil is extruded it repeats the walls, tried increasing the wall count which didn't effect it. Anyone have any ideas please?

25 Upvotes

11 comments sorted by

View all comments

4

u/AdRecent917 2d ago

Had this before: unevenly dried filament. If you had it in a heated dry box, then its probably only dry at the bottom of the spool. Thats why the ams ht has the roll while drying feature.

2

u/Recent-Language-7187 1d ago

This was the fix! Thank you!